How do I distinguish blocking from ink set-off?
Inspect both separated faces: transferred ink color indicates set-off, while sticking or loss of surface material indicates blocking or picking. More than one defect may be present. LK1022 is an inline aqueous OPV with an anti-blocking application claim; that claim does not remove the need to check drying and pile conditions.
Separate the sheets and look at both faces. Ink colour on the reverse of the next sheet is evidence of set-off. Sheets that resist separation or lose surface material also show blocking or picking. These defects can occur together. Photograph a dark solid and a lightly printed area so the press crew can locate the damage on the original artwork.
Which coater and pile conditions should I record first?
Record where sticking occurs, the wet deposit, board and ink lots, line speed, airflow, extraction and pile temperature. LK1022 lists 40±1% solids and 40±10 s viscosity, but the supplied seconds do not identify a cup method. Confirm that method in the TDS before interpreting a press-side viscosity reading.
- Check where it repeats. Compare samples from the top, centre and lower part of the pile and from each side of the sheet. Note whether sticking follows heavy ink coverage, spans the whole sheet or appears only after storage.
- Check water removal. Record the board and ink lots, coating deposit or anilox specification, line speed, airflow, extraction and dryer settings. A heavier wet deposit gives the dryer more water to remove. Compare the settings with the last good run on that stock.
- Measure heat where the sheets sit. Record the pile temperature with the same sensor at comparable positions and times. A hotter dryer can leave more heat in the pile. Inspect cooling and exhaust before increasing the heat setting.
How can I separate a drying problem from a stacking problem?
Split sheets from one run between the normal pile and a smaller lift, keeping the contact faces and inspection time consistent. Record pile temperature, height and load. If both groups stick, change one drying or coating variable within the approved process range, then verify the result at the normal production pile height.
On a trial, split sheets from the same run into the normal delivery pile and a smaller lift. Keep the same faces in contact. Record stack height, temperature, elapsed time and any applied load. Compare separation, colour transfer and gloss marks at the time the job would normally go to finishing. A difference points to pile conditions worth investigating.
If both groups stick, keep the stacking conditions fixed and change one drying or coating variable within the supplier’s operating guidance. Repeat the comparison. Confirm the improvement at normal production pile height before releasing the job.
Product values are typical ranges from the supplied specifications. Use the latest grade-specific TDS/SDS and documented substrate trials for production approval. A stated benchmark is not a result measured on your construction.